==Notes==
+
{{needspics}}
These are various notes culled from threads on the Hotrodders Bulletin Board and related links. Needs to be organized and verified.
+
[[Image:Rust at battery tray old versus new.JPG|thumb|300px|A rusted battery tray alongside a new one.]]
 +
==What is rust and its causes?==
 +
Rust is a kind of corrosion/burning -- a decay or breakdown of a material in reaction to its environment. Specifically, rust is an electrochemical corrosion that occurs in the presence of iron, oxygen, and water. Oxygen and water are available in the open air, and iron is the principal ingredient in steel.
  
 +
For rust to occur it needs an anode (a piece of metal that gives up electrons), an electrolyte (a liquid that helps transport electrons), and a cathode (a piece of metal that accepts electrons). The more conductive the electrolyte, the quicker rust will occur. For this reason, humid air, salty air, or salty water will accelerate the formation of rust.
  
===Cause of rust===
+
Iron, with the chemical symbol of Fe, combines with oxygen, O, to form Fe<sub>2</sub>O<sub>3</sub>, the chemical formula for common reddish-brown rust. In its mineral form, Fe<sub>2</sub>O<sub>3</sub> is known as hematite.
Need more background here. Plus info on why newer cars don't rust nearly as badly, and on salt/winter driving conditions. Review this article: http://www.metalwebnews.com/howto/rust/rust.html .
+
  
 +
Rust is commonly referred to as ''iron oxide''.  An oxide is a type of chemical compound that contains oxygen and other elements (like nitrous oxide, N<sub>2</sub>O). Oxides are typically formed when elements come into contact with air, through a process known as oxidation. Oxides are common, comprising most of the earth's crust. Elements can have multiple oxides. For example, there are sixteen known iron oxides. Thus, it's more accurate to say that rust is '''an''' iron oxide, rather than saying that rust '''is''' iron oxide.
  
===Media blasting rust===
+
Other metals besides iron oxidize, but their oxidation is not referred to as rust. For example, when aluminum oxidizes, it forms a protective, corrosion-resistant coating that is similar in appearance to un-oxidized aluminum. Zinc oxidizes similarly, which is why it is used for galvanizing. Only the oxidation of iron and steel is known as "rust". Why? Because iron oxide takes up more physical space than iron. It's bigger. So, when iron and air combine to make Fe<sub>2</sub>O<sub>3</sub>, it "puffs out", exposing even more of the original steel to the elements.
*Sand is not recommended for media blasting panels. It acts like little hammers, warping panels with by compressive forces (analagous to hail). Use softer media (list examples): 55 grit silica-based media.
+
Can be done, but must be cautious. Use a small sandblaster, or a sandblaster set on low (expand on this: distance, angle, etc.).
+
*Can sandblasting "increase" rust? Or, if the rust is removed and the metal is sealed, shouldn't it be eliminated? Some thoughts on this are:
+
**Although sandblasting may appear to have removed all the rust to the naked eye, it hasn't really done so.
+
**It's caused by water in the air compressor line, as sand will harbor some moisture. Also, compressed air contains moisture. And, sand has salt in it. A moisture trap in the line should solve the problem with the water in the air line.
+
*Many panels have seams, hems, and bends that are inaccessible by blasting, and hold moisture and rust.
+
*Body panels can be sand blasted. However, it must be done carefully (explain). The pressure of the sand hitting the body panels causes warpage.
+
*One option is to use chemical paint stripper, then use a sandblaster to lightly "dust" the remaining rust.
+
*Media blasting can remove good metal from body panels too. Also, used media can have metal particles left in the media.
+
*Soda blasting can remove light rust, and won't warp panels.
+
*[http://en.wikipedia.org/wiki/Sugar_sand Sugar sand] is finer and less-damaging than regular sand.
+
*For cleaning in seams, a spot blaster is recommended.
+
* Take precautions with proper safety equipment (list it here)
+
  
===Accessing rust between interior panels===
+
There is another iron oxide also referred to as "rust". It's Fe<sub>3</sub>O<sub>4</sub>, commonly called "black oxide", or, in mineral form, magnetite. This is the stuff that's left over after using certain products to "convert" rust. Black oxide takes up the same amount of space as iron, so it doesn't bulge it out, like reddish-brown rust, Fe<sub>2</sub>O<sub>3</sub>. Since black oxide itself doesn't offer much protection against corrosion, it's typically covered up (often with [[epoxy primer]]). Black oxide is an example of a conversion coating, a metal coating where part of the surface is converted into the coating itself, by a chemical or electrochemical process.  
Pressure washer with pencil tip can knock everything loose out.
+
  
Drill small holes, get a spray wand with a 360-degree head. Then, when done, weld the holes shut.
+
===Why do older cars rust more than newer cars?===
 +
*Cars are more aggressively coated these days. Galvanizing (explain).
 +
*Steel used in cars is of a higher quality these days.
 +
*More salt is used on roads these days.
 +
*Progressive evolution of engineered 'self rinsing' technology, such as strategically designed/placed  drain holes to allow rain or wash water to purge body cavities of moisture absorbing rust producing sediments, moreover, robotic assembly methods to lessen the possibility of human error which may compromise the operation of such a design by 'less than precise' assembly. eg; the human worker adds an over-sized glob of body filler next to a fender well drain hole which inadvertently clogs it, causing the fender well to hold moisture laden debris instead.
 +
*Electrolysis due to some older cars (British) having 'positive ground' electrical systems -where the car's electrical system is basically all 'ground wires' instead. (eg: AMC Metropolitan assembled by Austin Motor Company in Longbridge, England -neither were they dipped in a rust preventing primer bath, then they were shipped in ocean salt air to be sold in USA)
  
 +
=Rust assessment=
  
===What exactly is e-coating?===
+
==The "best" way to handle rust==
 +
The "best" way to do something often implies the existence of the "best" conditions in regard to skill, time, and money.
  
===Getting your entire body acid dipped===
+
For example, the "best" way to handle anything more than surface rust on body panels is to liberally cut out the rusted area, and weld in a patch panel. Ideally, any metal shaping and metal finishing should be done without the use of any body filler products whatsoever. Many people don't have the necessary skill to do this.
About $1000 - $1500? From Redi-Strip (technically not an acid? research this), a national chain.
+
  
===POR-15, Zero-Rust, Eastwood Rust Encapsulator===
+
The "best" way to handle surface rust on an entire body is to have it professionally dipped, often at a cost of over $1000. This amount of money may not be available for a specific project, or it may be impractical to invest it.
These might be the top 3?
+
  
Len Stuart of Autobodystore.com recommends Picklex-20 followed by Zero Rust: http://www.autobodystore.com/new_page_1.htm
+
If you take time to properly assess your own rust situation, you can choose a well thought-out solution that's "best" for you.
  
from Eastwood: [http://www.eastwoodco.com/jump.jsp?itemID=852&itemType=CATEGORY&iMainCat=688 Rust encapsulator v. POR-15]
+
==Areas to assess==
  
Topcoat these products? Some may have a UV-resistant clearcoat to go with them -- research it.
+
===The rusted part or piece===
 +
*Can the part be removed? How large is it? Is it small enough to be soaked?
 +
*What part is it? Is it a body panel?
  
===The fiberglass resin patch trick===
+
===The rust itself===
One technique that has been recommended is to grind/clean the rust, tape the underside of the panel to be patched, and then fill the holes with fiberglass resin, then paint and undercoat. This trick is not a good idea -- when the body flexes, there will be cracks in the fiberglass pieces.
+
How bad is it? Exactly how to assess:
  
===Surface rust removal technique===
+
*Jab rusty areas with a screwdriver, scratch awl, or icepick, and see if they go through.
Need 80-180 grit sandpaper, DA sander (or sand by hand), steel wool, naval jelly, squirt bottle w/warm soapy water, and paper towels.
+
*After cleaning rust off of floor pans, wait until it's dark, and put a trouble light under your car. Pinholes in the sheet metal will show up very well in such a situation.
 +
*Rust coming through seams? (research this)
  
#Get all heavy rust off with DA sander and 80-180 grit paper.
+
===Climate and operating environment===
#Working in 1-2 square feet at a time, wearing rubber gloves, scrub with naval jelly and steel wool. Don't let the naval jelly dry, keep it wet, squirt with bottle.
+
Do you live in a climate where water or salt will be present in the air? Is it a wintery climate where snow and/or salt will be present on the roads? Near the ocean?
#Rinse and re-apply naval jelly if necessary, to get to clean shiny metal.
+
#When finished with an area, wipe off excess naval jelly with paper towel, squirt on warm soapy water, and dry thoroughly. Then wipe down with lacquer thinner. Can then sand with 180 grit. After that, you can just use wax and grease remover, and then paint with epoxy primer.
+
  
Can use seam sealer afterwards on seams. SEM #39777.
+
What environment will the part be operating in? Interior of car? Undercarriage? Submerged in oil?
  
===Quick fix for exposed areas (dents, etc.)===
+
===Skills===
If a dent causes an area of bare metal to be exposed. To "hold" it so it won't rust until a paint job is ready to be done: gently bump out the dent, sand, rattle can primer, rattle can sealer.
+
Most of the skills required for removing rust are commonplace. However, certain jobs may require welding, or metal shaping.
  
 +
===Tools===
 +
Besides basic hand tools, do you have an air compressor? Access to a DA sander? Angle grinder with wire wheel? Media blaster? Spot blaster? Blast cabinet? Spray gun? In some cases electric powered tools can be used instead of pneumatic tools.
  
===How to seal insides of doors?===
+
===Cost===
 +
How much money do you have to put into the rust removal? What's the value of the project? Are you doing it "for money or for love"? If you plan on selling the project, can you expect a reasonable return on your investment?
  
===Examining rust===
+
===Time===
After cleaning off rust of floor pans, wait until it's dark, and put a trouble light under your car. Pinholes in the sheet metal will show up very well in such a situation.
+
How much time can you put into the project? Both work time, and wait time. Do you have the time necessary to eliminate surface rust from a body by hand? Do you have time to drop a part into a bucket, and wait a few weeks while it soaks?
  
Jab rusty areas with a screwdriver, scratch awl, or icepick, and see if they go through.
+
===Overall vehicle plan===
 +
What's your overall plan for the vehicle with the rusted part or piece? What kind of abuse is it going to take, and how important are looks? Will it be a daily driver? Are you going to show it?
  
===Patch panels===
+
=Rust removal, treatment, and prevention=
Butt weld or lap weld?
+
  
Importance of weld-through primer?
+
==Chemicals and finish products==
  
 +
===Understanding "magic formula" marketing===
 +
The market for rust removal, conversion, and encapsulation products is rife with far-fetched claims of "secret formula" rust solutions.
  
===Soda blasting?===
+
Realistically, it's not very difficult for one company to chemically analyze another company's "secret formula", and produce an identical (or extremely similar) product. Many of the various rust removal and encapsulation products are, more or less, the same. A lot of it boils down to marketing, and the situation is only exacerbated by the fact that it's difficult to make a thorough assessment of a rust treatment product.  Properly assessing a rust treatment solution would likely involve waiting several years, and then removing any outer layers of finish so that any existing underlying rust could be examined.
  
===Preventing flash rust===
+
The uneducated consumer will likely recoil at the abundance of "magic" formulas for treating rust, and revert to selecting a safe, well-known, name-brand product line. This is a reasonable solution for many, but the name-brand rust treatment products tend to be rather expensive, especially in consideration of the fact that they are often comprised of inexpensive, common chemicals.
Especially, if you're not doing all of your bodywork at once.
+
Recommended: Eastwood metal wash,  
+
  
 +
Someone who has achieved good results with a certain combination of rust treatment products will often stay loyal to their method, without exploring other potential options that may indeed provide better results at a lower cost.
  
===Electronic Rust Inhibition===
+
===Miscellaneous (need to be sorted)===
*[http://www.counteractrust.com/ CounterAct Electronic Rust Protection]?
+
*[http://www.tat-co.com/product.asp?ID=154 Body-Tec amber rustproofing]. 24 oz spray can. manufac: " Light viscosity allows material to flow into hard to reach areas easily. Ideal for core supports, sheet metal, frames etc"
*[http://www.ruststopnorthamerica.com/electronic-rustproofing-rust-proofing.htm Rust Stop North America]
+
*[http://www.d-rust-it.com D-Rust-It] -- available in concentrate.
 +
*Amsoil HD
 +
*Slicksand
 +
*Featherfill
 +
*[http://www.krylon.com/main/product_template.cfm?levelid=5&sub_levelid=13&productid=1789&content=product_details Krylon rust tough primers]
 +
*[http://www.rustbeeter.com RustBeeter] (made from beets, maybe it's like molasses?)
 +
*Duro Extend
 +
*Devoe Bar-Rust
 +
*[http://www.noxudolusa.com/rust_protection/Rust_Protection.html Noxudol]
 +
*Loctite Extend Rust Treatment
 +
*Rustoleum (generally considered a poor choice for automotive applications. Good for cheap shop shelving, etc.)
 +
*[http://www.permatex.com/products/automotive/specialized_maintenance_repair/body_interior_trim/auto_Permatex_Rust_Treatment.htm Permatex Rust Treatment]
 +
*[http://ridrust.com/ RidRust]
 +
*[http://solutions.3m.com/wps/portal/3M/en_US/3MAutomotive/Aftermarket/Products/Product-Catalog/?PC_7_0_53BC_root=GST1T4S9TCgv&PC_7_0_53BC_output=html&PC_7_0_53BC_gvel=6DTWTJQPBBgl&PC_7_0_53BC_vroot=GSLPLPKL4Xge&PC_7_0_53BC_node=GSQJ0YVJLSbe&PC_7_0_53BC_theme=en_US_aad_portal&PC_7_0_53BC_command=CustomizePageHandler Rust Fighter]
 +
*DuPont 5717S Metal Conditioner
 +
*[http://www.rustx.com/ Rust-X]
 +
*[http://www.jasco-help.com/products/prod_mg.htm Jasco]
 +
*Prep-sol
 +
*[http://www.napasco.com/enrustreat.htm Mar-Hyde Rust Converter]
 +
*Rust N-M-E
 +
*[http://www.penntoolco.com/catalog/products/products.cfm?categoryID=2182 Knorrostol]
 +
*[http://www.hammerite-automotive.com/ Hammerite]
 +
*[http://www.eurekafluidfilm.com/ Fluid Film]
 +
*[http://www.waxoyl.com/en/produkte/120-4.htm Waxoyl]
 +
*[http://rustonic.com Rustonic]
 +
*[http://duplicolor.com/products/rustfix.html Duplicolor Rust Fix]
 +
*[http://www.therustdoctor.com/ Rust Doctor]
 +
*[http://bluelightning.zoovy.com/product/RR32 Blue Lightning]
 +
*[http://www.picklex20.com Picklex-20]
 +
*[http://rust007.com/knockout.htm Rust Knockout]
 +
*[http://www.napasco.com/enrustreat.htm Enrust]
 +
*[http://rust007.com/destroyerhome.htm Rust Destroyer]
 +
*Rust-Check
 +
*[http://www.evaporust.com/ Evapo-Rust Rust Remover]
 +
*[http://www.safestrustremover.com/ Safest Rust Remover]
 +
*[http://www.corroless.com/ Corroless]
 +
*[http://www.kleanstrip.com/special.htm Klean Strip Rust Converter]
 +
*[http://www.zerorust.com/ Zero Rust] -- [http://www.zerorust.com/tech.htm tech page], [http://www.zerorust.com/faq.htm faq]. Rust cleaning product is "prep-step", and clearcoat is called "crystal coat".
 +
*Rust Reformer
 +
*[http://www.rustbullet.com Rust Bullet]
 +
*[http://www.ospho.com/ Ospho]
 +
*Oxisolve
 +
*Rust-n-me
 +
*DuPont Metal Conditioner
 +
*PPG Metal Prep
 +
*DuPont Vari-Prime
 +
*All-Metal
 +
*[http://tntrustremover.com/ TNT Rust Remover]
  
===Penny trick for filling holes===
+
===Rust removers and "converters"===
Grind down all the paint and rust from around the hole. Clamp a piece of copper to the other side (roof flashing, etc.). Then, fill in the hole with a MIG welder. When done, unclamp the copper -- it won't stick to the panel. Also, it absorbs the heat, so the panel won't warp as much.
+
After using an acid to remove rust, flush the surface with water and baking soda '''(confirm or expand on this)'''.
  
Will brass work too?
+
When converting/neutralizing rust:
 +
# Get everything off first that you can by sanding and wire brushing (wire brushing will get into the pits better).
 +
# A rust converter/neutralizer containing tannic acid, phosphoric acid or another type of acid should be used
 +
# Be careful of getting this stuff on your concrete floor as it will bubble and decompose it.
 +
# Follow the instructions on the bottle when you are done there should be a fine coating on the metal which will help prevent further rust from developing.
 +
# This stuff is hard on paintbrushes (eats away the bristles) and you must be very careful of your eyes. Also it will ruin paint, so, again, use caution.
  
What about drilling and patching pinholes?
+
Lots of "rust neutralizers/metal etchers/floor etchers/metal conditioners" contain primarily phosphoric acid, which reacts with rust (iron oxide) to create iron phosphate, a hard black substance over which primer can be applied.
  
===Removing rust from chrome===
+
Don't use battery acid (sulfuric acid) or muriatic acid (hydrochloric acid) for rust removal. Strong acids are dangerous, and there are many more effective chemicals.
Use a mag wheel polish.
+
*[http://www.ospho.com/ Ospho] Manufacturer description: When applied to rusted surfaces, it resists/retards rust in chemical change on drying to a tough, hard surface ready for priming.
 +
*[http://rustbeeter.com/ Rustbeeter] Merchant description: A byproduct of the sugar refining process. Probably similar to molasses. Parts must be submerged. Parts soak in a bucket for usually under a week, but as long as several weeks. Food product. Dry powder that gets mixed with water. Non-acidic or caustic. After use, parts are cleaned with dish soap and water, dried, and coated.
 +
*[http://www.tinmantech.com/html/must_for_rust_remover_inhibi.php Must for Rust] Merchant description: removes rust and corrosion, non-caustic to skin, needs no neutralizing, primer goes right over it. $28/gallon.
 +
*[http://www.eastwoodco.com/shopping/product/detailmain.jsp?itemID=15974&itemType=PRODUCT&iMainCat=373&iSubCat=374&iProductID=15974 Eastwood Rust Converter] Merchant description: 2-part mix, adheres to bare or rusty steel, and can be top coated with most coatings. 1 gallon each of the 2-part mix is $125.
 +
*[http://www.rust-cure.com/ Rust Cure] Merchant description: phosphoric acid-based. leaves a thin film that bonds well with most primers and paints. for pricing, need to see this page: http://rustcure.bizland.com/xwheretobuy.html .
 +
*[http://www.eastwoodco.com/jump.jsp?itemID=1124&itemType=PRODUCT Oxisolv Rust Remover] Merchant description: dissolves rust and leaves behind a zinc phosphate coating. Spray/brush/dip. Non-toxic, non-flammable, and re-usable. Must be cleaned off before priming.
 +
*[http://www.eastwoodco.com/jump.jsp?itemID=11122&itemType=PRODUCT Eastwood Rust Dissolver] Merchant description: acid free rust remover, leaves surface ready to paint, plate, or powder coat. Suitable for engine parts, and harmless to copper, brass, aluminum, solder, lead, plastic, rubber, seals, wood or vinyl. Surface must remain wet for product to work. $40/gallon.
 +
*[http://sem.ws/product.php?product_id=164 Rust-Mort] Merchant's description: "Converts rust to a black or grayish, hard, insoluble, protective coating".
 +
*[http://sem.ws/product.php?product_id=206 SEM Rust-Seal] Manufacturer description: "Transforms rust leaving a tough, permanent, black protective coating. RUST-SEAL can be left exposed or may be top coated with enamels, lacquers or urethanes."
  
 +
''(Make sure that none of the above count as "encapsulators". Also, what about the converters that leave a "protective film" on the metal. They say that they don't need neutralization, and they don't need to be washed off. Is this as good as cleaning to bare metal, and then hitting with epoxy primer?)''
  
===Electrolysis===
+
*Vinegar
Removing rust with electrolysis -- research this: http://www.stovebolt.com/techtips/rust/electrolytic_derusting.htm .
+
*Muriatic acid (not for use on body panels, as it causes [http://en.wikipedia.org/wiki/Hydrogen_embrittlement hydrogen embrittlement])
 +
*Toilet cleaner (?)
 +
*Cola (yes, contains phosphoric acid)
 +
*Phosphoric acid: leaves behind a coating of iron phosphate
 +
*Naval jelly (gelled phosphoric acid)
 +
*Mag wheel cleaner (?)
 +
*Molasses (a 1:10 solution of molasses to water can be used for soaking rusty parts, although it loses its strength after several months)
 +
*Powdered household cleaning products such as Comet or Ajax
  
===Undercoatings===
+
===Rust encapsulators===
Rubberized undercoatings?
+
''Main article: [[Rust encapsulators]]''
  
*There are many different products and approaches for handling rust.
+
Rust encapsulators work by sealing off existing rust, denying it the oxygen it needs to grow.
*Rust encapsulators are common in the hotrodding industry. Some people think that they won't get rid of a problem, and may make it worse. Oftentimes its is how you apply and prepare it.
+
*A common thought is that minor surface rust of body panels is treatable, but everything else must be cut out and replaced with new metal. However, this is not always true. But some seriously bad rust you will have too replace.
+
  
===Plasma spray welding===
+
The use of rust encapsulators in hotrodding is controversial. Hotrodders typically divide into 3 distinct camps over the use of rust encapsulation products on vehicles:
With plasma spray welding, metal wire is converted to sprayable form, and used to repair rust holes, fill panel joints, and blend patch panels. One example is the machine sold by [http://www.rustbustersllc.com Rustbusters].
+
  
===How to clean engine water jackets or radiator of rust===
+
#Won't use rust encapsulation products at all.
Flush with CLR, Kool Klean (can't find). Manufacturers of CLR say that it shouldn't be used in a radiator: http://www.jelmar.com/CLRbasic.asp .
+
#Will use rust encapsulation products, but not on body panels.
 +
#Will use rust encapsulation products on a variety of parts, including body panels.
  
When building an engine, to prevent rust: when done washing it and blowing it dry, oil it down, and store it in a plastic bag -- sealed (confirm this).
+
===Rust preventive oils and waxes===
 +
*[http://www.brownells.com/aspx/NS/store/ProductDetail.aspx?p=1134 Cosmoline] . "Cosmoline" is a trade name for a generic rust preventative which conforms to US military specification MIL-C-11796C. It's a soft, brushable grease that's commonly used for preserving and storing firearms. "Rated to protect polished steel panels from rust for one year in open shed storage, and 30 days, minimum, in a humidity cabinet." $30/gallon
 +
*[http://boeshield.com/index.htm Boeshield T-9] "Designed to penetrate metal pores and dissolve minor corrosion, then leave a resilient waxy coating that lasts for many months." $100/gallon
 +
*[http://www.eastwoodco.com/jump.jsp?itemID=1117&itemType=PRODUCT Eastwood Heavy-Duty Anti-Rust]. Merchant's description: spray-on brown wax film which forms an air and water-tight barrier. won't crack, flake, or peel. used for inside door panels, or to protect bare metal parts during storage. $15/quart
 +
*[http://www.oxisolv.com/html/long_term.html Oxisolv rust inhibitor long term] -- Merchant description: displaces water on metal parts to prevent rust. environmentally safe, bio-degradable, protects steel. Apply by spraying thoroughly, or dipping.
 +
*[http://sem.ws/product.php?product_id=161 SEM internal panel coating] Manufacturer description: "provides corrosion protection to inner body panels and other metal parts"
 +
*[http://solutions.3m.com/wps/portal/3M/en_US/3MAutomotive/Aftermarket/Products/Product-Catalog/?PC_7_0_53BC_root=GST1T4S9TCgv&PC_7_0_53BC_output=html&PC_7_0_53BC_gvel=6DTWTJQPBBgl&PC_7_0_53BC_vroot=GSLPLPKL4Xge&PC_7_0_53BC_node=GS3H3CPLMLbe&PC_7_0_53BC_theme=en_US_aad_portal&PC_7_0_53BC_command=CustomizePageHandler 3M Rust Fighter application wand]
 +
*[http://solutions.3m.com/wps/portal/3M/en_US/3MAutomotive/Aftermarket/Products/Product-Catalog/?PC_7_0_53BC_root=GST1T4S9TCgv&PC_7_0_53BC_output=html&PC_7_0_53BC_gvel=6DTWTJQPBBgl&PC_7_0_53BC_vroot=GSLPLPKL4Xge&PC_7_0_53BC_node=GSQJ0YVJLSbe&PC_7_0_53BC_theme=en_US_aad_portal&PC_7_0_53BC_command=CustomizePageHandler 3M Rust Fighter]
 +
*[http://enjenjoesproducts.com/cg020001.html Brownpolymer rust inhibitor long term] -- Merchant description: displaces water on metal parts to prevent rust. environmentally Safe,It's a Cleaner,It's a Polish,It's a Lube, It's a Grease,It's a Protective Coating,Multi Use Polymer Substance
 +
*You can make your own basic rust protection coating from 1 part anhydrous lanolin (available from a pharmacy), and 5 parts paint thinner.
 +
*For machine tools, this is recommended: http://www.clclubricants.com/waylubes.htm .
 +
*Use something that releases rust-inhibiting vapor. Rust-blox vapor tabs, vpi paper, permatex in-charge corrosion inhibitor.
  
===Surface rust===
+
===Epoxy primer===
Just sand with a DA, apply rust neutralizer, clean thoroughly, and prime.
+
''Main article: [[Epoxy primer]].''
  
===Rust pitting===
+
Epoxy primer/sealer is a non-porous finish that is typically recommended as the first basecoat over bare steel. Various epoxy primers can also be applied over [[Fiberglassing|fiberglass]], plastic, or the black iron phosphate coating that remains after "converting" rust.
After removing all surface rust, treat with metal prep, wash, dry, sand, prime, fill the pits with polyester putty (or Evercoat's Metal 2 Metal), then smooth and prime again.
+
  
A spot blaster is useful for this: silica as the medium. Grinding wheel, die grinder.
+
Epoxy primer is a two-part mix, with a hardener that has to be added before spraying. Body fillers and high-build primers can be used on top of epoxy primer.
  
Or, repeatedly prime with a high build primer and block sand. You may have to prime/block several times to get the pitted area up to the same level as the surface around it.
+
===Seam sealers===
 +
Seam sealers are used to seal roof channels, drip rails, trunk seams, door seams, and other body seams. They can be either one or two-part, and are typically applied over primer, sometimes with the use of a specially-designed caulking gun or spray gun.
  
Sprayable body filler, called "SlickSand"? From Evercoat? Like a "very high build primer"? Hard, but sands easy.
+
*Lord Corporation makes several seam sealers: [http://www.lord.com/Home/ProductsServices/Adhesives/FusorAutomotiveAftermarketProducts/Products/SealersFoams/tabid/3402/Default.aspx Lord Corporation sealers and foams].
 +
*3M manufactures several different types of seam sealers: [http://solutions.3m.com/wps/portal/3M/en_US/3MAutomotive/Aftermarket/Products/New-Products/?PC_7_0_5FJC_command=CustomizePageHandler&PC_7_0_5FJC_theme=en_US_aad_portal&PC_7_0_5FJC_output=html&PC_7_0_5FJC_vroot=GSLPLPKL4Xge&PC_7_0_5FJC_gvel=6DTWTJQPBBgl&PC_7_0_5FJC_node=GSWMS8NB1Nbe&PC_7_0_5FJC_root=GST1T4S9TCgv 3M seam sealers].
 +
*SEM Products makes a [http://sem.ws/Catalog.asp?prod=96 seam sealer], a [http://sem.ws/Catalog.asp?prod=271 beige seam sealer], a [http://sem.ws/Catalog.asp?prod=269 high build self-leveling seam sealer], and a [http://sem.ws/Catalog.asp?prod=98 self-leveling seam sealer].
 +
*Transtar Autobody Technologies makes a variety of seam sealers: [http://www.tat-co.com/productCategory.asp?ID=6#sub9 Transtar seam sealers].
 +
*International Epoxies and Sealers: [http://www.internationalepoxies.com/sealers.htm International Epoxies and Sealers body sealers].
 +
*Valvoline makes their [http://www.pliogripbyvalvoline.com/sealers_foam.html Pliogrip line of seam sealers].
 +
*Evercoat has the [http://www.evercoat.com/productCategory.aspx?cat=41 Maxim line of seam sealers].
 +
*McKanica makes a seam sealer in an aerosol can: [http://www.google.com/search?rls=en&q=mckanica+seam+sealer&ie=UTF-8&oe=UTF-8 McKanica seam sealer].
  
Let naval jelly sit on the pitted area overnight, if possible. Cover naval jelly with plastic wrap to keep it from drying out overnight.
+
====See also====
 +
[http://autobodystore.com/forum/showthread.php?t=7467 "Basics of Basics": Seam Sealers (by Brian Martin)]
  
===Removing surface rust===
+
===Metal washes, wax and grease removers===
*How about using baking soda and water?
+
*[http://www.eastwoodco.com/jump.jsp?itemID=258&itemType=PRODUCT&path=1%2C2%2C458%2C467%2C473&KickerID=39&KICKER Eastwood Metal Wash]. Merchant's description: dry compound that is mixed with water. removes grease and oils from bare metal, and leaves behind corrosion inhibitors that prevent flash rusting and promote paint adhesion. $11 for enough dry mix to make 7 quarts.
 +
*[http://www.aerospace.henkel.com/index.cfm?ID=178 Metalprep 79] Manufacturer's description: phosphoric acid-based cleaner. leaves surface chemically clean and corrosion free. thoroughly rinse with water when done. brush/spray/dip
 +
*Is DuPont's "Quick-Prep" equivalent to Metalprep?
  
*To remove surface rust, use naval jelly (jelled phosphoric acid) and steel wool.
+
Read this thread thoroughly: [http://www.hotrodders.com/forum/what-else-wax-grease-remover-besides-mineral-spirits-51150.html What to use to remove wax, etc.]
#Work in small areas, not larger than a square foot.
+
#Apply jelly with 000 steel wool, rub it in, and allow it to set for a couple of minutes. Don't let it dry.
+
#Rub again with steel wool. Repeat a few times, and then clean the area. Dry it immediately.
+
  
*To convert/neutralize rust
+
The following are not to be used as metal cleaners: lacquer thinner, acetone, reducers. Use the product within the recommendations of your product system. Cleaners typically vary as to strength, and time they take to evaporate.
# Get everything off first that you can by sanding and wire brushing (wire brushing will get into the pits better)
+
# A rust converter/neutralizer containing phospheric acid or another type of acid shold be used
+
# Be careful of getting this stuff on your concrete floor as it will bubble and decompose it
+
# Follow the instructions on the bottle when you are done there should be a fine coating on the metal which will help prevent further rust from developing
+
# This stuff is hard on paintbrushes(eats away the brisles) and you must be very careful of your eyes. Also it will ruin paint so again use caution.
+
  
===Gas tanks===
+
Use clean, purpose-designed paint rags for cleaning with cleaners.
Put a handful of nuts and bolts in, chain, chainsaw blade, etc., and shake it around a bit to knock out the loose stuff. Then, clean with muriatic acid. Pour it in, let it sit for up to an hour, then flush with water and baking soda to neutralize. Or, Eastwood has a kit for this: an acid to clean it, and then something to coat it with. However, some people say that the coating can clog up the fuel filter, or trash your OEM sending unit. The best way to do it is to take it out and get it re-tinned.
+
  
===Removing rust===
+
===Weld-through primer===
Shop vac, putty knife, metal brush, wire wheel on grinder for loose stuff, or wire wheel that fits on a drill (not as good as grinder).
+
Weld-through primer zinc-rich coating that conducts current from a welder, and doesn't burn off when welding. It can provide protection on lap welds and inner weld seams.Weld-through primer is often applied to the mating areas when welding body panels.
Phosphoric acid, muriatic acid, toilet bowl cleaner, naval jelly -- let it sit: 20 minutes, hours, overnight.
+
Coca-cola for rust removal?
+
After acid, flush with water and baking soda.
+
Lots of "rust neutralizers/metal etchers/floor etchers/metal conditioners" contain phosphoric acid. Turns the rust into a hard black substance.
+
Hit rust with a 60-grit sanding pad to make sure there is no rust left behind it.
+
  
*Start with as low as 36 grit, and finish with about 220.
+
*3M
*Scotch-brite pads and Comet/Ajax.
+
*U-Pol
*3M clean-n-strip disc?
+
*"silver" POR-15? Has a filler in it for minor imperfections?
+
  
*Some people mentioned that professional body shops don't use POR-15 or similar rust "encapsulators" because:
+
===Panel adhesives===
**They would have to re-do too much of their work.
+
Used to adhere body panels, as an alternative to welding. Need more information on these.
**Rust prevention products are primarily advertised in hobbyist mags, not in periodicals read by professionals in the paint and body industry.
+
**The lack of rust preventive products in non-hobbyist industries does appear suspect. For example, why don't ships at sea use POR-15?
+
**The major paint manufacturers like Sherwin Williams, PPG, and DuPont don't produce a POR-15 like product. This is thought to be because they couldn't possibly warranty such a product.
+
**The fact that POR-15 is not used by manufacturers is also important.
+
  
 +
==Tools==
 +
*Shop vac
 +
*Putty knife
 +
*Metal brush
 +
*Sand paper. 36 grit to 220 grit.
 +
*Wire wheel on drill. When the wire bristles start to bend one way, reverse the drill and work in the other direction for a while.
 +
*Wire wheel on grinder, or, these discs are considered to be superior to wire wheels: [http://solutions.3m.com/wps/portal/3M/en_US/Manufacturing/Industry/Product-Catalog/Online-Catalog/?PC_7_0_4UVL_root=GST1T4S9TCgv&PC_7_0_4UVL_output=html&PC_7_0_4UVL_gvel=H55CPWS904gl&PC_7_0_4UVL_vroot=81LC4NNTD4ge&PC_7_0_4UVL_node=RCM96XTX07be&PC_7_0_4UVL_theme=en_us_manufacturingindustry_portal&PC_7_0_4UVL_command=CustomizePageHandler 3M clean & strip disc], or [http://solutions.3m.com/wps/portal/3M/en_US/Marine/Home/Products/Catalog/?PC_7_0_4S4T_root=GST1T4S9TCgv&PC_7_0_4S4T_output=html&PC_7_0_4S4T_gvel=RJ5GMFSMV0gl&PC_7_0_4S4T_vroot=GS4JK4Y166ge&PC_7_0_4S4T_node=GSGKXWRKYVbe&PC_7_0_4S4T_theme=en_US_marineproducts_portal&PC_7_0_4S4T_command=AbcPageHandler 3M bristle disc], or [http://solutions.3m.com/wps/portal/3M/en_US/Marine/Home/Products/Catalog/?PC_7_0_4S4T_command=AbcPageHandler&PC_7_0_4S4T_theme=en_US_marineproducts_portal&PC_7_0_4S4T_output=html&PC_7_0_4S4T_vroot=GS4JK4Y166ge&PC_7_0_4S4T_gvel=RJ5GMFSMV0gl&PC_7_0_4S4T_node=GSVDY2CZYDbe&PC_7_0_4S4T_root=GST1T4S9TCgv Surface Conditioning Disc].
 +
*Scotch-brite pads
 +
*Steel toothbrush
 +
*Media blaster
 +
*Blasting cabinet
 +
*Spot blaster
 +
*Welder
 +
*Steel wool
  
To clean frames: wash with water, wire brush, heat with torch, wire brush again, sand blast, blow with compressed air, then hit with rust converter.
+
===Tips===
 +
*When using a wire wheel, don't sit in one spot for too long -- the localized heat from friction can warp sheet metal.
  
===Chemical dipping===
+
==Methods==
Complete acid dips are best, but expensive. By this method, the entire body is dipped into a tank.
+
===Body panel rust removal===
 +
Ideally, only surface rust on body panels is "treated". Anything more than that would mean that the affected area would be cut out, and replaced with fresh metal.
  
 +
====Removing surface rust from body panels====
 +
First, remove all the heavy surface rust with a DA sander and 80-180 grit paper.
 +
To remove surface rust, use naval jelly (jelled phosphoric acid) and steel wool.
 +
#Work in small areas, not larger than a square foot. Wear rubber gloves, and scrub with naval jelly and steel wool.
 +
#Apply jelly with 000 steel wool, rub it in, and allow it to set for a couple of minutes. Don't let it dry. Keep it wet, using a squirt bottle. For inclines, you can also soak some fabric in water, and lay it on the naval jelly.
 +
#Rub again with steel wool. Repeat a few times.
 +
#When finished, wipe off the excess naval jelly with a paper towel, squirt on warm soapy water, and dry thoroughly.
 +
#Wipe down with lacquer thinner.
 +
#Sand with 180 grit.
 +
#Use wax and grease remover, and then spray with epoxy primer.
 +
#From there, you can apply body filler (the epoxy may need to be scuffed, read instructions).
 +
#When the filler work is done, scuff with a red scotch-brite pad.
 +
#Then, apply two more coats of epoxy, followed by high-build primer.
  
 +
====Cutting out rust====
 +
First, make a tape template. Tape off the area that's going to be cut off, leaving a healthy border of good metal. Transfer the tape template to the patch panel, in one piece. Cut out the templated piece from the patch panel. Then, screw the cut-out piece to the car as a temporary guide. From there, rough-shape the patched piece. Cut some slits if necessary, and hammer. Then, make the cut on the body panel, with the patch still screwed to the car. Then, unscrew the panel from the car, and hammer-form it on a bench, anvil, etc. Finally, butt-weld it back onto the car. Weld, with lots of spread-out spot welds (wait for them to cool), so the panel doesn't warp. Then, grind down the welds. Treat with rust protection, then body filler, primer, etc.
  
Even high grade epoxies and finishes are not 100% impermeable to water and air.
 
  
===Evapo-Rust===
+
A quarter panel rust fix demonstrating the above is illustrated here: http://www.a2zautoforums.com/showthread.php?t=700
Interesting article here: http://www.stovebolt.com/techtips/rust/evaporust/index.html . Forum guy reviews evapo-rust. Disadvantages of acid: can't breathe it, must wash all parts thoroughly after using it, or the acid starts working again when it gets wet.
+
  
===Storing body panels===
+
 
Use epoxy primer (AKA epoxy primer/sealer), it won't allow rust. Not the same as regular primer.
+
====Treating light body rust (from storing panels) prior to epoxy====
 +
Sand with 80 grit, wash with wax and grease remover. Use waterborne wax and grease remover, instead of solvent-borne (research exactly what that means), let set 15-30 minutes. Dry with a blower and a tack rag. Spray epoxy.
 +
 
 +
====Getting the entire vehicle body dipped====
 +
''(Need more info on Redi-Strip. What chemical do they use? What's the cost? Can a hobbyist acquire and use the same chemical that Redi-Strip uses? When the body is returned to you, is it truly completely clean, or does it have to be cleaned to get all of the chemical removed from nooks and crannies, etc.?)''
 +
 
 +
====Quick fix for exposed areas (dents, etc.)====
 +
If a dent causes an area of bare metal to be exposed. To "hold" it so it won't rust until a paint job is ready to be done: gently bump out the dent, sand, rattle can primer, rattle can sealer.
 +
 
 +
====Do both sides of a panel have to be treated with rust converter/encapsulator?====
 +
Explain this.
 +
 
 +
====Removing pitted rust in body panels====
 +
See: [[pitted rust]].
 +
 
 +
====Fixing rust holes in body panels====
 +
See: [[pitted rust]].
 +
 
 +
====Storing body panels====
 +
Use epoxy primer (aka "epoxy primer/sealer"), it won't allow rust. Not the same as regular primer.
 
Wet-sand down to 400 grit, wash/dry, grind down rust to bare metal, apply body filler where needed, blow off, clean with prep-sol or similar cleaner, tape it up, and prime with epoxy primer.
 
Wet-sand down to 400 grit, wash/dry, grind down rust to bare metal, apply body filler where needed, blow off, clean with prep-sol or similar cleaner, tape it up, and prime with epoxy primer.
  
Do epoxy primers need a topcoat?
+
====Removing rust in seams====
 +
A spot blaster is useful.
  
Is epoxy primer the best coating for bare metal?
+
To do it right, you will generally need to pull the seam apart, remove the rust, and then hit it with a rust conversion product. However, sometimes you can open up the layers slightly with a hammer and putty knife used between the spotwelds. Bend the flange open, media blast into the seam, clean, prime with epoxy primer, brush in urethane seam sealer, and close the seam back up. If the seam is not accessible, flood it with a penetrating cavity wax, like 3M's Rustfighter.
  
No, you can't get epoxy primer in a rattle can. It's a two-part mix, with a hardener that has to be added before you spray it.
+
====Accessing rust between interior panels====
 +
Pressure washer with pencil tip can knock everything loose out.
  
===Various commercial rust encapsulators and rust removers (need to be sorted)===
+
Drill small holes, get a spray wand with a 360-degree head. Then, when done, weld the holes shut.
POR-15 is expensive. Are there other products that are just as good, but not so pricey? One problem with using "rust coating products" is that, for hobbyists, it's often best to stick with a single line of paint/finish products, from bare metal to clearcoat. Using most rust products means that you're outside of the product line for the rest of the finish. So, it may be physically incompatible (resulting in a poor paint job), or it may void the product warranty.
+
  
*[http://www.rustoleum.com/brand.asp?frm_brand_id=41&SBL=5 Rustoleum Tremclad]
+
Turn panels around to slosh rust remover around. Blow compressed air inside the panel.
*[http://www.rust-cure.com/ Rust Cure]
+
*[http://www.boeshield.com/ Boeshield]
+
*[http://www.eastwoodco.com/shopping/product/detailmain.jsp?itemID=16408&itemType=PRODUCT&iMainCat=373&iSubCat=374&iProductID=16408 Eastwood Rust Encapsulator]
+
*[http://www.eastwoodco.com/jump.jsp?itemID=1117&itemType=PRODUCT Eastwood Heavy-Duty Anti-Rust]
+
*[http://www.eastwoodco.com/jump.jsp?itemID=258&itemType=PRODUCT&path=1%2C2%2C458%2C467%2C473&KickerID=39&KICKER Eastwood Metal Wash]
+
*[http://www.eastwoodco.com/shopping/product/detailmain.jsp?itemID=15974&itemType=PRODUCT&iMainCat=373&iSubCat=374&iProductID=15974 Eastwood Rust Converter] (converts rust to inert black oxide)
+
*[http://www.eastwoodco.com/jump.jsp?itemID=1124&itemType=PRODUCT Oxisolv Rust Remover]
+
*[http://www.eastwoodco.com/jump.jsp?itemID=11122&itemType=PRODUCT Eastwood Rust Dissolver]
+
*Amchem Metalprep
+
*Duro Extend
+
*[http://solutions.3m.com/wps/portal/3M/en_US/3MAutomotive/Aftermarket/Products/Product-Catalog/?PC_7_0_53BC_root=GST1T4S9TCgv&PC_7_0_53BC_output=html&PC_7_0_53BC_gvel=6DTWTJQPBBgl&PC_7_0_53BC_vroot=GSLPLPKL4Xge&PC_7_0_53BC_node=GSQJ0YVJLSbe&PC_7_0_53BC_theme=en_US_aad_portal&PC_7_0_53BC_command=CustomizePageHandler Rust Fighter]
+
*DuPont 5717S Metal Conditioner
+
*[http://www.jasco-help.com/products/prod_mg.htm Jasco]
+
*[http://www.napasco.com/enrustreat.htm Mar-Hyde Rust Converter]
+
*Rust N-M-E
+
*[http://www.hammerite-automotive.com/ Hammerite]
+
*[http://www.eurekafluidfilm.com/ Fluid Film]
+
*Waxoyl
+
*[http://rustonic.com Rustonic]
+
*[http://duplicolor.com/products/rustfix.html Duplicolor Rust Fix]
+
*[http://www.therustdoctor.com/ Rust Doctor]
+
*[http://bluelightning.zoovy.com/product/RR32 Blue Lightning]
+
*Picklex-20
+
*[http://rust007.com/knockout.htm Rust Knockout]
+
*[http://www.napasco.com/enrustreat.htm Enrust]
+
*[http://rust007.com/destroyerhome.htm Rust Destroyer]
+
*Rust-Mort
+
*Rust-Check
+
*[http://www.evaporust.com/ Evapo-Rust Rust Remover]
+
*[http://www.corroless.com/ Corroless]
+
*[http://www.kleanstrip.com/special.htm Klean Strip Rust Converter]
+
*[http://www.zerorust.com/ Zero Rust] -- [http://www.zerorust.com/tech.htm tech page], [http://www.zerorust.com/faq.htm faq]. Rust cleaning product is "prep-step", and clearcoat is called "crystal coat"
+
*Rust Reformer
+
*[http://www.rustbullet.com Rust Bullet]
+
*[http://www.ospho.com/ Ospho]
+
*Oxisolve
+
*Rust-n-me
+
*DuPont Metal Conditioner
+
*PPG Metal Prep
+
*DuPont Vari-Prime
+
*Recommended body filler is All-Metal. Thought to be more moisture-resistant.
+
(are some rust "converters" really just muriatic acid?)
+
  
===Rustproofing brake rotors===
+
Cut hole in panel? Spray rust killer with garden sprayer?
Zinc dip, also Eastwood has some solutions?
+
  
===Muriatic acid is another name for hydrochloric acid===
+
A mirror can be used to check areas for rust.
  
===Patching frames===
+
Don't spray expanding foam. It absorbs water, and will cause more rust. It can also expand and cause the panels to push out.
Usually not worthwhile, unless it's a special or valuable frame. Too easy to replace, and too much potential structural damage. Has to be done perfectly. Can be replaced with steel of the same gauge as the original frame, and welded in to place.
+
  
Where is the rust on the frame? In a critical stress area? How bad is it?
+
====How to treat rusty drip-rails?====
 +
#blast
 +
#wash with wax and grease remover
 +
#spray with 2 coats of epoxy
 +
#spray with seam sealer
 +
 
 +
====Plasma spray welding====
 +
With plasma spray welding, metal wire is converted to sprayable form, and used to repair rust holes, fill panel joints, and blend patch panels. One example is the machine sold by [http://www.rustbustersllc.com Rustbusters].
 +
 
 +
====Rusted window channels====
 +
''(Difficult to fabricate, need more info on this.)''
 +
 
 +
===Vinyl tops===
 +
Rust is common in vinyl tops. The vinyl gets porous after a few years, and lets in moisture.
 +
 
 +
''(How to prevent?)''
 +
 
 +
Vaseline ,push it in between the moldings around the top and wipe off excess.Spray a heavy oil around Landau /opera windows let sit and wipe off excess any little tears should also have a drop of silicone pushed in them to avoid moisture.
 +
 
 +
===Leaf spring rust===
 +
Remove rust, then, ideally, paint them separately. Re-assemble with teflon strips.
 +
 
 +
===Preventing rust at chassis to ground connection===
 +
Silicone dielectric grease, electrical bonding paste; spray well with clear lacquer after bonding the connection.
 +
 
 +
===Cleaning light surface rust off crankshaft===
 +
 
 +
Have a machine shop polish the journals.
 +
 
 +
May require a regrind to the next correct bearing size prior to polishing depending on tolerances.
 +
 
 +
Using a decent regular flow of CRC 5.56 or a PTFE type spray and an M3 grey scotchy (then try green scotchbrite if need) rubbed in direction of crank travel, localised to effected area. Mask off area with masking tape to prevent scratching unaffected areas if necessary.
 +
 
 +
Rust is tough, and large areas vigourously rubbed (mechanically or otherwise) may cause damage to the finish of the journal. Initial contact needs to be with clean CRC rinsed rag, keep the journal area clean and use a light touch, buffing in one direction until the initial rust colour no longer shows.
 +
 +
If sand paper is to be employed, try starting with 2000 grit (no less than 1200 grit), change paper regularly, and keep the strokes light. You are only removing the outer scale, you are not resurfacing the journal just rubbing out rust.
 +
 +
Phosphoric acid localised can help in any pits.
 +
 
 +
Acids on hardened steels can cause embrittlement so dont leave it on long, only enough to blacken the rust. Afterwards switching to a microfibre rag with a product like Autosol, Blue Magic or even Brasso, you can polish out any minor scratches on the journal. Steel wool usually isn't recommended as it can scratch the journal finish, and it creates fine particles that must be throuoghly cleaned from the crank. If rust is more than 0.005" deep get it resurfaced.
 +
 
 +
Also-
 +
 
 +
* Very fine steel wool or scotchbrite pad, and light oil. Rub around the journals in the direction of rotation, not across.
 +
* Cut 600 grit wet or dry sandpaper into strips the width of the crank journals. Wrap it around the journal, and secure it with tape. Then, make a strap from leather, about one-half the width of the sandpaper strips. Use the strap on the paper in a shoeshine motion. Finish off with some light oil on the sandpaper. Do a few strokes first, then clean the paper, because the rust will clog the sandpaper.
 +
 
 +
''(LP3 as rust inhibitor on crankshafts?)''
 +
 
 +
===Electrolysis===
 +
Advantages: self-limiting (can't remove too much), safe (low electrical current), won't harm good metal, not an acid (less dangerous, and no risk of hydrogen embrittlement)
 +
 
 +
Need: a plastic tub, iron electrode, water and washing soda (sodium carbonate), and a batter charger. About 1 tablespoon of soda per gallon of water. Can't find washing soda, then lye will work. Wear eye protection and protect skin too. Connect the electrode to the positive battery terminal. Connect the rusted object to the negative terminal. Submerge the object. Make sure the contact is good (may need to clean off some of the rust from the rusty part). Typically takes a few hours, but can take up to overnight. Rinse or scrub with brush to remove final rust debris. May need to re-treat. Oil, wax, or prime soon after. Surface of rusted metals is black after treatment.
 +
 
 +
Be creative to clean oddly-shaped objects:
 +
 
 +
*plastic PVC pipes
 +
*large 2x4 wood boxes lined with plastic sheeting
 +
*suspend an electrode in a cavity
 +
*use a sponge soaked in the electrolyte solution, with a backing electrode, for objects that can't be submerged.
 +
 
 +
The powder used is a mild alkali.
 +
 
 +
====Resources====
 +
*[[Electrolytic rust removal]] Crankshaft Coalition wiki article
 +
*http://www.stovebolt.com/techtips/rust/electrolytic_derusting.htm
 +
*http://hotrodders.com/forum/rust-removal-lower-arms-other-suspension-parts-108384.html
 +
*http://www.davidbradley.net/ERR.html
 +
*http://antique-engines.com/trailer-electrolysis.htm
 +
*http://www3.telus.net/public/aschoepp/electrolyticrust.html
 +
*http://www.fordmuscle.com/forums/other-articles/467718-rust-removal-electrolysis.html
 +
*http://www.hotrodders.com/forum/electrolytic-rust-removal-revisited-163423.html
 +
 
 +
===How to remove rust from chrome===
 +
*Mag wheel polish, or [http://www.turtlewax.com/main.taf?p=2,1,4,12 Turtle Wax Chrome Polish].
 +
*Fine steel wool, scotch-brite pads, crumpled-up pieces of aluminum foil.
  
 
===Preventing engine rust===
 
===Preventing engine rust===
 
Engine storage spray, or wipe down with [http://www.marvelmysteryoil.com/ Marvel Mystery Oil].
 
Engine storage spray, or wipe down with [http://www.marvelmysteryoil.com/ Marvel Mystery Oil].
  
Cylinder walls with flash rust: marvel mystery oil, steel wool, etc. Pitted rusting will necessitate a rebuild.
+
Cylinder walls with flash rust: Marvel Mystery Oil, steel wool, etc. Pitted rusting will necessitate a rebuild.
  
===Frame rust===
+
===How to de-rust gas tanks===
Sandblasting or dipping is best. Then, wire wheel is next-best. Can be professionally sandblasted and powder-coated for ~$250 at a good price.
+
Put a handful of nuts and bolts in, chain, chainsaw blade, etc., and shake it around a bit to knock out the loose stuff. Not too aggressive -- you'll dent the tank. Then, clean with phosphoric acid. Pour it in, let it sit for up to an hour, then flush with water and baking soda to neutralize. Or, Eastwood has a kit for this: an acid to clean it, and then something to coat it with. However, some people say that the coating can clog up the fuel filter, or trash your OEM sending unit. The best way to do it is to take it out and get it re-tinned.
  
For minor surface rusting, with mostly metal showing through, it's OK to just powder-coat it.
+
===How to clean engine water jackets or radiator of rust===
 +
Flush with CLR, Kool Klean (can't find). Manufacturers of CLR say that it shouldn't be used in a radiator: http://www.jelmar.com/CLRbasic.asp .
  
===After removing rust===
+
When building an engine, to prevent rust: when done washing it and blowing it dry, oil it down, and store it in a plastic bag -- sealed ''(confirm this)''.
Need to wash and prep surface, with a solvent like lacquer thinner or DuPont Prep-Sol.
+
  
===Removing rust encapsulators from skin===
+
==="Oiling" your car===
Soak in vegetable oil for 30 minutes, or use a solvent (is there a specific POR-15 solvent?).
+
In climates that are more prone to rust, cars are sometimes "oiled". Rocker panels, doors, and other body passages are drilled and sprayed inside with oil, used oil, or gelled oil substances. Entire frame and suspension are also oiled. Can be done yearly in very rust-prone climates.
  
===Rusted window channels===
+
Historically, this procedure has been used before driving the car down a dirt road. The dirt sticks to the oil on the underside of the vehicle, providing an effective sealing layer. Consider how, when removing a dirty, oily gasket, the metal beneath it is clean. Same concept.
Bad news. Difficult to fabricate.
+
  
 +
Now, this might be done with an application-specific undercarriage wax or oil.
  
===Quick spot repairs===
+
===Preventing MIG wire rust===
What if you have a small area of metal exposed? Can you use a spray can quick-fix? Or prep, shoot, clean with a gun?
+
Store in a bag with some dessicant packets. Here's a list of dessicants: [http://en.wikipedia.org/wiki/List_of_desiccants List of dessicants]. Also, can use small old refrigerator with 100 watt bulb inside, for storing rods and wires. Stays about 100 degrees. Small fan inside too.
  
 +
===Underside rust removal===
 +
Best not to do this as overhead work. Tilt the car on a rotisserie, or raise it significantly overhead.
  
===Cleaning the inside of a boxed, open-ended frame===
+
Another option is to keep the car low to the ground, and, with plastic sheeting and duct tape, seal the area between car and floor. Leave the rear area of the plastic "tent" open for access. At the front of the "tent", affix a shop vac hose (exhaust). Blast.
 +
 
 +
===Rustproofing brake rotors===
 +
Zinc dip, also Eastwood has some solutions? Research this.
 +
 
 +
===Axle tube rust===
 +
When rebuilding a rear end, the rust can be cleaned out with naval jelly/shoving rags down it with a broomstick.
 +
 
 +
===Cleaning hand tools===
 +
Tumble in a cement mixer with oil and sand. Or, soak in a bucket with parts cleaner or paint thinner.
 +
 
 +
===Rust prevention on tools===
 +
Keep tools in a wooden toolbox. Also, use a shop dehumidifier. Avoid dust on your tools, as it can attract moisture, and thus, rust.
 +
 
 +
===Electronic rust inhibition===
 +
*[http://www.counteractrust.com/ CounterAct Electronic Rust Protection]?
 +
*[http://www.ruststopnorthamerica.com/electronic-rustproofing-rust-proofing.htm Rust Stop North America]
 +
 
 +
''(This is known as [http://en.wikipedia.org/wiki/Cathodic_protection cathodic protection]. Research this. And: [http://en.wikipedia.org/wiki/Sacrificial_anode sacrificial anode] and [http://en.wikipedia.org/wiki/Galvanic_anode galvanic anode].)''
 +
 
 +
===Frame rust===
 +
Sandblasting or dipping is best. Then, stripping wheel or wire wheel is next-best. Can be professionally sandblasted and powder-coated for ~$250 at a good price.
 +
 
 +
Patching is usually not worthwhile, unless it's a special or valuable frame. Too easy to replace, and too much potential structural damage. Has to be done perfectly. Can be replaced with steel of the same gauge as the original frame, and welded in to place.
 +
 
 +
Where is the rust on the frame? In a critical stress area? How bad is it?
 +
 
 +
For minor surface rusting, with mostly metal showing through, it's OK to just powder-coat it.
 +
 
 +
OR:
 +
 
 +
#blast/wire wheel
 +
#phosphoric acid
 +
#clean off acid with thinner
 +
#etching primer
 +
#epoxy primer
 +
 
 +
====Cleaning the inside of a boxed, open-ended frame====
 
Blow out all the dirt, etc. Then, attach a strong towel to some strong cord. Soak the towel with rust treatment chemical, and pull it through the frame.
 
Blow out all the dirt, etc. Then, attach a strong towel to some strong cord. Soak the towel with rust treatment chemical, and pull it through the frame.
  
===Rivets, fiberglass patches, body adhesive glue===
+
===Media blasting rust===
For when you can't weld. Fiberglass patches are temporary solutions. Rivets are definitely not the way to go. What about body adhesive glue?
+
See: [[Media blasting]].
  
===Step-by-step epoxy primer application to panels===
+
*Sand is not recommended for media blasting panels. It acts like little hammers, warping panels with compressive forces (analagous to hail). It can be done, but extreme caution must be used. Sand also dulls as it is used, which reduces its cutting efficiency with each reuse.
#strip, and sand with 80-grit sandpaper
+
*Use softer media (list examples):
#clean with wax and grease remover until a clean towel can be rubbed on it without discoloring
+
**55 grit silica-based media
#spray 2 coats of epoxy, according to manufacturer's directions
+
**[http://en.wikipedia.org/wiki/Sugar_sand Sugar sand] is finer and less-damaging than regular sand.
#body filler can be applied next, although sometimes the epoxy will need to be scuffed or sanded (read instructions)
+
*Can sandblasting "increase" rust? Or, if the rust is removed and the metal is sealed, shouldn't it be eliminated? Some thoughts on this are:
#when the filler work is done, scuff the whole panel with a red scotch-brite pad.
+
**Although sandblasting may appear to have removed all the rust to the naked eye, it hasn't really done so.
#then, apply two more coats of epoxy, followed by high-build primer.
+
**It's caused by water in the air compressor line, as sand will harbor some moisture. Also, compressed air contains moisture. And, sand has salt in it. A moisture trap in the line should solve the problem with the water in the air line.
 +
**Sand by hand after sandblasting, to eliminate this issue.
 +
*Many panels have seams, hems, and bends that are inaccessible by blasting, and can hold moisture and rust. A spot blaster is recommended.
 +
*One option is to use chemical paint stripper, then use a sandblaster to lightly "dust" the remaining rust.
 +
*Media blasting can remove good metal from body panels too. Also, used media can have metal particles left in the media.
 +
*Soda blasting can remove light rust, and won't warp panels. However, when soda blasting body panels, the resultant film can negatively affect finish adhesion. For more details, see: [[Soda blasting]].
  
===Treating rusted body panels===
+
=Miscellaneous=
First, rust must be removed: chemicals, blasting, sanding, or cutting it out and replacing with fresh metal. If you can't completely remove it, you'll need to use a rust converter or a rust encapsulator.
+
  
With converters and encapsulator, be sure to treat rust from both sides of the panel.
+
==Flooded vehicles==
 +
Flooded vehicles can be very difficult to handle, as there can be rust in any and all places. They are best avoided, unless it's the car that you really want.
  
*Why do older cars rust more quickly? Theories are:
+
==What's galvanization?==
**Cars are more aggressively coated these days. Galvanizing (explain).
+
''(needs confirmation)''
**Steel used in cars is of a higher quality these days.
+
**More salt is used on roads these days.
+
  
===Axle tube rust===
+
"Galvanizing" typically refers to hot-dip galvanizing, a process by which iron or steel is coated with a thin layer of zinc, by dipping it in a molten bath of zinc. Galvanized steel can be welded. It's been used for more than 150 years.
When rebuilding a rear end, the rust can be cleaned out with naval jelly/shoving rags down it with a broomstick.
+
  
 +
Zinc oxidizes when exposed to air, forming zinc oxide, which then reacts with water molecules in the air to form zinc hydroxide, which then reacts with carbon dioxide in the air to form zinc carbonate. Zinc carbonate (the final "galvanizing" layer), is a thin but very tough protective layer. It also acts as a "sacrificial anode". It will corrode before the steel it is protecting.
  
===How to treat rusty drip-rails?===
+
Many modern automotive body panels are galvanized.
#sand blast
+
 
#wash with wax and grease remover
+
You can buy cold galvanizing spray. ''(list examples here)''
#spray with 2 coats of epoxy
+
#spray with seam sealer
+
  
 +
==Hydrogen embrittlement==
 +
All acids contribute hydrogen to metal. This causes hydrogen embrittlement, which weakens the metal. Untrue: you can "bake" the hydrogen out at 400 degrees F, after exposing a metal to acid.
  
How to apply seam sealer/cavity wax?
+
==Fiberglass resin patches==
 +
One technique that has been recommended is to grind/clean the rust, tape the underside of the panel to be patched, and then fill the holes with fiberglass resin, then paint and undercoat. This trick is not really a good idea -- when the body flexes, there will be cracks in the fiberglass pieces. Metal also expands at different rates than [[Fiberglassing|fiberglass]], causing cracks to form, allowing more rust to form in these cracks.
  
===Pitting===
+
Using POR-15 (a moisture-cured urethane) and fiberglass cloth will produce a low-cost repair that will bond and flex with the metal. In fact, POR-15 sells a $20 kit to do this very thing. While this method does fill the holes and provides a rust-resistant repair, it does not restore any mechanical strength to the metal like an actual metal patch panel would.
Naval jelly and wire wheel, many iterations.
+
  
When done, sand with 80 grit, clean, and coat with epoxy primer.
+
==Do metal etches leave coating?==
 +
Follow up on metal etches like DuPont's Metal Etch or POR's Metal Ready leaving a phosphoric acid coating on the metal that will prevent flash rusting while storing.
  
 +
==How to remove rust protection==
 +
How to remove old rust protection finishes? Or undercoating?
  
===Mag wheel cleaner as rust remover?===
+
*Wire wheel
 +
*Brake cleaner
 +
*Kerosene
 +
*Heat gun
 +
*EZ-Off oven cleaner
 +
*Mineral spirits
 +
*Freeze with dry ice, then chisel out
 +
*Wallpaper steamer
  
===Cosmoline===
+
==What about riveting in patch panels?==
What about [http://www.brownells.com/aspx/NS/store/ProductDetail.aspx?p=1134 Cosmoline] for short-term rust prevention (up to one year) on parts? Also, drilling holes in inaccessible parts (frames), and filling with Cosmoline?
+
Very low-end solution, like [[fiberglass]] patching metal. Panel adhesives are a better choice when you can't weld.
  
===Bulk notes===
+
=Resource dump=
*Phosphoric acid (naval jelly, etc.) reacts with rust (iron oxide), to form iron phosphate (the black stuff that naval jelly leaves behind). Neutralize with: baking soda.
+
'''Drop links in here if they're relevant to this article. They'll be reviewed, incorporated, and referenced.'''
*Muriatic acid (hydrochloric acid) is for cleaning aluminum, not steel. Don't use it on body metal! Causes hydrogen embrittlement.
+
*[http://www.carcraft.com/howto/24544/ CarCraft article on using POR-15 and fiberglass mat for hole repair]
*Don't ever use battery acid (sulfuric acid) to remove rust. Very dangerous to work with, and harms metal.
+
*[http://lasertronics.com/ Lasertronics.com]
*To keep naval jelly wet, soak some fabric in water, and lay it on the naval jelly. Can work on an incline.
+
*[http://www.theruststore.com/rust_info.aspx articles at theruststore.com]
*What grit sandpaper to use when removing rust from body panels?
+
*http://www.corrosionsource.com/index.htm
*Holes must be cut out, and new metal welded in.
+
*[http://www.fertanamerica.com/ Fertan rust remover]
*Using straight hydrochloric (same as muriatic) acid requires that it be properly neutralized (how to do this?), otherwise there is a risk of hydrogen embrittlement causing cracks in thinner areas of sheet metal.
+
*[http://en.wikipedia.org/wiki/Galvanization Galvanization]
*Don't sit in one spot too long with a wire brush -- it will warp the metal.
+
*[http://www.safestrustremover.com/ SafestRustRemover.com]
*The iron phosphate coating that's left behind by rust converter is a fine base for primer.
+
*[http://www.instructables.com/id/E17UQMY28PEQ6T2A5Z/?ALLSTEPS Electrolytic rust removal]
*To remove rust, wire brush, or wire wheel the area. Also: [http://solutions.3m.com/wps/portal/3M/en_US/Manufacturing/Industry/Product-Catalog/Online-Catalog/?PC_7_0_4UVL_root=GST1T4S9TCgv&PC_7_0_4UVL_output=html&PC_7_0_4UVL_gvel=H55CPWS904gl&PC_7_0_4UVL_vroot=81LC4NNTD4ge&PC_7_0_4UVL_node=RCM96XTX07be&PC_7_0_4UVL_theme=en_us_manufacturingindustry_portal&PC_7_0_4UVL_command=CustomizePageHandler 3M clean & strip disc], or [http://solutions.3m.com/wps/portal/3M/en_US/Marine/Home/Products/Catalog/?PC_7_0_4S4T_root=GST1T4S9TCgv&PC_7_0_4S4T_output=html&PC_7_0_4S4T_gvel=RJ5GMFSMV0gl&PC_7_0_4S4T_vroot=GS4JK4Y166ge&PC_7_0_4S4T_node=GSGKXWRKYVbe&PC_7_0_4S4T_theme=en_US_marineproducts_portal&PC_7_0_4S4T_command=AbcPageHandler 3M bristle disc]
+
*[http://www.hotrodders.com/forum/good-durable-paint-frame-98391-2.html rust protection paint]
*POR-15 shouldn't be used on parts that will see direct sunlight -- it's color will change (although it won't lose its anti-rust capabilities).
+
*http://counteractrust.com/
*POR-15 can't be applied over primer. Has to be done per instructions.
+
*http://en.wikipedia.org/wiki/Pickling_%28metal%29
*POR-15 is largely considered a "duct tape fix" or a "git-er-done" solution. It may be OK for the home hobbyist, but it's not considered the "right way" or the "professional way" to handle rust.
+
*http://en.wikipedia.org/wiki/Pickle_liquor
*When using wire wheel on drill, when the wire bristles start to bend one way, reverse the drill and work in the other direction for a while.
+
*[http://www.finishing.com/116/94.shtml e-coating]
*Brands: POR-15, Zero Rust, Eastwood Rust Encapsulator. These are NOT rust "converters", they don't alter rust, etc. There is a common misconseption that the ones listed are converters, but that is in fact false. They are a coating intended to seal out air and moisture.  
+
*http://www.novelindia.com/Stainless_Steel_Pickling_Passivation_Chemical.htm
*Another argument against rust "treatments" is that many of them require the surface to be lightly rusted first. "Inducing" rust seems wrong to people.
+
*[http://www.metalwebnews.com/howto/rust/rust.html rust primer]
*Rust-protection products can either act as a coating, or as a sacrificial anode (explain).
+
*[http://www.theruststore.com/rust_info.aspx rust removal and prevention articles]
*If POR-15 and similar products have a "lifetime warranty", explain how guarantees like that don't involve labor costs, losses, or other related costs.
+
*[http://www.tinmantech.com/html/faqs.php#rust rust faqs and info]
*One recommendation is: after sandblasting, remove some more of the surface metal by sanding with sandpaper. This is done to remove the salt, sand, moisture, etc. from the surface.
+
*[http://antique-engines.com/electrol.asp rust removal by electrolysis]
*After preparing panels, coating them with epoxy primer is recommended.
+
*[http://www.rowand.net/Shop/Tools/Electrolysis.htm rust removal]
*Phosphoric acid or muriatic acid are recommended as well.
+
*[http://www.stovebolt.com/techtips/rust/electrolytic_derusting.htm electrolytic rust removal]
*Rust forms so quickly that if you are sand blasting, media blasting, etc., the surface rust will begin to form before you finish the job.
+
*[http://www.brownells.com/aspx/NS/store/ProductDetail.aspx?p=1134 Cosmoline]
*Molasses is thought to work, but takes a while. 1 part molasses to 10 parts water.
+
*http://www.jasco-help.com/products/prod_mg.htm
*To remove rust: Comet/Ajax with Scotch-Brites, and then muriatic acid with scotch-brites, and then rinse and wash with Comet/Ajax again to neutralize the acid.
+
*[http://www.restorick.com/tech/topic.asp?TOPIC_ID=37 zero rust application tips]
*POR-15 is a three-step process: degreaser, then metal prep, then POR-15 paint. (verify this).
+
*[http://www.clausenautobody.com/proddetail.php?prod=rust-defender Rust defender product]
*What's "all-metal"? Same as all-metal prep?
+
*[http://www.hotrodders.com/forum/master-chemical-nomorerust-pitted-surfaces-154053.html Hotrodders Bulletin Board rust discussion]
  
Links to review: http://www.tfhrc.gov/pubrds/novdec98/laboratory.htm , http://www2.sherwin-williams.com/im/cs/cs-spring2003/feature-01.asp .
+
=Related resources=
 +
*[http://www.sizes.com/tools/sandpaper.htm Sandpaper sizes]
 +
*[http://solutions.3m.com/wps/portal/3M/en_US/Manufacturing/Industry/Product-Catalog/Abrasives/ 3M industrial abrasives]
 +
*[http://assist.daps.dla.mil/quicksearch/basic_profile.cfm?ident_number=9324 US military specification covering Cosmoline]
 +
*[http://en.wikipedia.org/wiki/Rust Rust]
 +
*[http://en.wikipedia.org/wiki/Corrosion Corrosion]
  
==References==
+
=References=
 +
*[http://www.metalwebnews.com/howto/rust/rust.html MetalWeb Rust Primer]
 +
*[http://www.bhi.co.uk/hints/rust.htm Electrolytic Rust removal FAQ]
 +
*http://en.wikipedia.org/wiki/Galvanization
 +
*http://en.wikipedia.org/wiki/Hematite
 +
*http://en.wikipedia.org/wiki/Magnetite
 +
*http://en.wikipedia.org/wiki/Conversion_coating
 +
*http://en.wikipedia.org/wiki/Iron_oxide
 +
*[http://science.howstuffworks.com/question445.htm How does rust work?] HowStuffWorks.com
 +
*[http://www.a2zautoforums.com/showthread.php?t=700 Quarter panel rust fix], ''A2Z Automotive Forums'', March 26, 2002.
 
*[http://www.hotrodders.com/forum/rust-what-acceptable-permanent-ways-get-rid-47303.html Acceptable ways to handle rust], ''Hotrodders Bulletin Board'', September 7, 2004.
 
*[http://www.hotrodders.com/forum/rust-what-acceptable-permanent-ways-get-rid-47303.html Acceptable ways to handle rust], ''Hotrodders Bulletin Board'', September 7, 2004.
 
*[http://hotrodders.com/forum/rust-pits-39.html Rust pits], ''Hotrodders Bulletin Board'', November 27, 2001.
 
*[http://hotrodders.com/forum/rust-pits-39.html Rust pits], ''Hotrodders Bulletin Board'', November 27, 2001.
Line 409: Line 620:
 
*[http://hotrodders.com/forum/rust-removal-trick-maybe-64839.html Rust removal trick], ''Hotrodders Bulletin Board'', June 26, 2005.
 
*[http://hotrodders.com/forum/rust-removal-trick-maybe-64839.html Rust removal trick], ''Hotrodders Bulletin Board'', June 26, 2005.
 
*[http://hotrodders.com/forum/gettin-old-rusty-spring-back-prime-shape-65335.html Getting an old rusty spring back to prime shape], ''Hotrodders Bulletin Board'', July 6, 2005.
 
*[http://hotrodders.com/forum/gettin-old-rusty-spring-back-prime-shape-65335.html Getting an old rusty spring back to prime shape], ''Hotrodders Bulletin Board'', July 6, 2005.
 +
*[http://hotrodders.com/forum/rust-around-vinyl-top-66610.html Rust around the vinyl top], ''Hotrodders Bulletin Board'', July 24, 2005.
 +
*[http://hotrodders.com/forum/cure-rusty-tank-67703.html A cure for rusty tank], ''Hotrodders Bulletin Board'', August 8, 2005.
 +
*[http://hotrodders.com/forum/cleaning-old-rusty-tools-68221.html Cleaning old rusty tools], ''Hotrodders Bulletin Board'', August 15, 2005.
 +
*[http://hotrodders.com/forum/rust-proofing-oil-72414.html Rust proofing with oil], ''Hotrodders Bulletin Board'', October 19, 2005.
 +
*[http://hotrodders.com/forum/new-have-question-about-panel-rust-repair-76001.html Question about panel rust repair], ''Hotrodders Bulletin Board'', December 12, 2005.
 +
*[http://www.hotrodders.com/forum/hmmm-rust-removal-answer-please-77479-2.html Rust in flooded cars], ''Hotrodders Bulletin Board'', December 30, 2005.
 +
*[http://hotrodders.com/forum/best-way-clean-rust-chrome-78043.html Best way to clean rust from chrome], ''Hotrodders Bulletin Board'', January 6, 2006.
 +
*[http://hotrodders.com/forum/wirewheeling-rust-79024.html Wirewheeling rust], ''Hotrodders Bulletin Board'', January 16, 2006.
 +
*[http://hotrodders.com/forum/rust-pitting-82402.html Rust pitting], ''Hotrodders Bulletin Board'', February 22, 2006.
 +
*[http://hotrodders.com/forum/magic-rust-removers-82287.html Magic rust removers?]' ''Hotrodders Bulletin Board'', February 21, 2006.
 +
*[http://hotrodders.com/forum/what-spray-sandblasted-steel-kill-rust-79237.html What to spray on sandblasted steel to kill rust?] ''Hotrodders Bulletin Board'', January 19, 2006.
 +
*[http://hotrodders.com/forum/fixing-rust-between-seams-85445.html Fixing rust between seams], ''Hotrodders Bulletin Board'', March 27, 2006.
 +
*[http://hotrodders.com/forum/removing-some-kind-rust-protection-86799.html Removing rust protection], ''Hotrodders Bulletin Board'', April 13, 2006.
 +
*[http://hotrodders.com/forum/how-remove-rust-under-car-floor-87359.html How to remove rust from under car floor], ''Hotrodders Bulletin Board'', April 19, 2006.
 +
*[http://spi.forumup.org/about156-spi.html Soda blasting], ''SPI Users Forum'', February 25, 2006.
 +
*[http://hotrodders.com/forum/surface-rust-inside-door-89225.html Surface rust on inside of door], ''Hotrodders Bulletin Board'', May 12, 2006.
 +
*[http://hotrodders.com/forum/rust-pits-89610.html Rust pits], ''Hotrodders Bulletin Board'', May 17, 2006.
 +
*[http://hotrodders.com/forum/how-treat-light-body-rust-prior-epoxy-89957.html How to treat light body rust prior to epoxy], ''Hotrodders Bulletin Board'', May 21, 2006.
 +
*[http://hotrodders.com/forum/preventing-rust-ground-chasis-connections-90035.html Preventing rust at ground to chassis connections], ''Hotrodders Bulletin Board'', May 22, 2006.
 +
*[http://hotrodders.com/forum/rusteeeed-inside-outside-98470.html Rusted from the inside or outside], ''Hotrodders Bulletin Board'', September 18, 2006.
 +
*[http://hotrodders.com/forum/mig-wire-rust-103305.html MIG wire rust], ''Hotrodders Bulletin Board'', November 26, 2006.
 +
*[http://hotrodders.com/forum/cleaning-rust-off-crankshaft-106495.html Cleaning rust off crankshaft], ''Hotrodders Bulletin Board'', January 11, 2007.
 +
*[http://hotrodders.com/forum/surface-rust-prep-before-paint-question-again-94158.html Surface rust prep before paint], ''Hotrodders Bulletin Board'', July 20, 2006.
 +
*[http://hotrodders.com/forum/quick-question-about-rustoleum-97198.html Quick question about Rustoleum], ''Hotrodders Bulletin Board'', September 2, 2006.
 +
*[http://hotrodders.com/forum/solution-preventing-all-rust-96594.html Solution to preventing all rust?], ''Hotrodders Bulletin Board'', August 26, 2006.
 +
*[http://hotrodders.com/forum/save-your-rusty-floor-board-108056.html Save your rusty floor board], ''Hotrodders Bulletin Board'', February 1, 2007.
 +
*[http://hotrodders.com/forum/hard-reach-rust-104414.html Hard to reach rust], ''Hotrodders Bulletin Board'', December 13, 2006.
 +
*[http://hotrodders.com/forum/stopping-rust-inside-103320.html Stopping rust from the inside], ''Hotrodders Bulletin Board'', November 26, 2006.
 +
*[http://hotrodders.com/forum/rust-treatment-repair-109939.html Rust treatment and repair], ''Hotrodders Bulletin Board'', February 25, 2007.
 +
 +
[[Category:Body and exterior]]
 +
[[Category:Good articles]]
 +
[[Category:Garage and shop]]
 +
[[Category:General hotrodding]]
 +
{{youcanedit}}

Latest revision as of 19:51, 4 February 2018